Field glossary · measurement
Strength test
In concrete acceptance, a strength test is a grouped result, not a count of cylinder breaks. Two qualifying cylinders at 4,700 and 4,900 psi produce one 4,800 psi strength test. ACI CODE-318-25 permits two standard-cured 4 by 8 in cylinders or two standard-cured 6 by 12 in cylinders; ACI 318-19 requires three when using 4 by 8 in cylinders. Identify curing, size, age and governing edition before forming the groups, then give each strength test equal weight in the rolling average.
The average of the cylinders in one set, broken at the designated age
Two small cylinders are permitted under the 2025 code
ACI CODE-318-25 Section 26.12.1.1(a) permits at least two standard-cured cylinders of either 4 by 8 in or 6 by 12 in size for one strength test. ACI's January 2026 Concrete Q&A confirms the change. ACI's cylinder-size guidance identifies the earlier ACI 318-19 requirement of three 4 by 8 in cylinders, so the project edition must remain visible in the sampling plan.
A project specifying ACI 301-20 still calls for three 4 by 8 in cylinders even though ACI 318-25 permits two. ACI's cylinder-size guidance explicitly identifies that specification requirement. Put the governing minimum in the sampling plan and reserve separate specimens for other ages and purposes; revising the code reference alone does not revise the contract's test schedule.
Average test results before calculating a rolling average
Equal weighting belongs to the strength tests, not to every cylinder in the report. Where valid tests contain different numbers of cylinders, flattening all individual breaks into one average weights the more heavily sampled test more strongly. Keep a sample identifier and a test identifier as separate fields in the laboratory export.
For three same-class tests using the 2025 minimum-cylinder basis, calculate the grouped values below before forming the rolling average. They average 4,300 psi. Flattening all seven breaks into one calculation produces 4,200 psi because the lowest-strength sample contributed an extra cylinder. That changes the weighting, not the concrete's performance.
| Strength test | Companion cylinder results | Test result |
|---|---|---|
| A | 4,700 and 4,900 psi | 4,800 psi |
| B | 3,500, 3,600 and 3,700 psi | 3,600 psi |
| C | 4,400 and 4,600 psi | 4,500 psi |
Test-method scope and technician qualification still apply
ASTM C39/C39M-26 limits its cylindrical concrete compression method to concrete denser than 50 lb/ft3 [800 kg/m3]. A low-density insulating material's reported strength therefore needs its applicable method identified instead of entering the structural-cylinder series under a generic 'strength test' label.
ASTM C39/C39M-26 also requires acceptance-testing personnel to meet ASTM C1077 technician requirements, including a performance examination evaluated by an independent examiner. Retain that qualification with the laboratory's test scope. A machine-generated load and strength printout establishes neither the specimen's eligibility for the test nor the technician's qualification to produce an acceptance result.
Distinctions
- Casting set
- A sample can supply specimens for several ages and purposes. The number cast is not the number averaged for each acceptance result.
- Field-cured construction-stage result
- ACI 318-25 treats this separately from the standard-cured acceptance strength test. Preserve individual field-cured values for the applicable release criterion.
Frequently asked questions
Can I combine a 7-day and a 28-day break into one strength test?
No. They describe different test ages. Keep each designated-age group under its own result and use the specified acceptance age for the acceptance series.
Sources checked
Also defined as
- Datacenter: The average of at least two 6x12 cylinders or three 4x8 cylinders from the same sample, broken at the specified age