ANVILFIELD Try FieldOS

Field glossary · property

Drying shrinkage

Drying shrinkage is reported as strain: measured loss of gauge length divided by its starting length after the chosen curing period. VTRC report 00-R1 cites 0.04% to 0.08% for typical unreinforced concrete, equivalent to 400 to 800 microstrain. A C157 result also needs its drying duration and conditioning history; those details let an estimator compare mixtures without treating specimen shortening as a predicted crack width.

The volume loss as concrete dries, driven by water content and paste, that the curl is built from

Used across 2 Anvilfield field guides, most in Concrete.
Updated

Convert percent shrinkage into movement

Virginia Transportation Research Council report 00-R1 identifies 0.04% to 0.08% as a typical drying-shrinkage range for unreinforced concrete. That is 400 to 800 microstrain, or 0.0004 to 0.0008 unit of shortening per unit of original length. Keep the percent sign in the calculation until the percentage has been divided by 100.

For a 20-foot length, that range corresponds to 0.096 to 0.192 inch of free shortening. Restraint changes how that movement appears: friction, reinforcement, and attached construction distribute it among elastic strain, joint movement, and cracks. The length-change calculation establishes a movement scale, not the width of a particular crack.

Reported shrinkageEquivalent strainFree shortening over 20 feet
0.04%400 microstrain0.096 inch
0.06%600 microstrain0.144 inch
0.08%800 microstrain0.192 inch

Read the conditioning history on a C157 report

ASTM C157/C157M-24e1 measures laboratory length changes caused by mechanisms other than externally applied load and temperature change, under controlled temperature and moisture conditions. The result is most useful when comparing mixes tested with the same preparation and exposure history.

ASTM C157/C157M-24e1 requires departures from its specified mixing, curing, sampling, or storage conditions to be prominently reported with the comparator results. A number labeled C157 is therefore incomplete evidence until its conditioning notes have been read. A supplier's modified drying program and a contract's standard program can produce different values for the same concrete.

In VTRC's 1999 study, shrinkage specimens received 28 days of moist curing at 23°C before drying at 50% relative humidity and 23°C. Those conditions explain the test's exposure; they do not describe an outdoor slab cycling through rain and sun. The published study followed shrinkage to 64 weeks, giving a much longer observation period than an early mix-submittal result.

Compare mixtures at the same drying age

Put specimen age and drying duration in different columns. A reading taken 28 days after casting is not equivalent to one taken after 28 days of drying when the specimens first spent time in moist storage. Also retain the reference reading and gauge length so a reported percent can be checked against the measured change.

For a floor complaint, keep the mixture's laboratory curve beside dated joint-opening and elevation measurements from the installed slab. The curve supports mixture comparison; the field record locates movement in the actual floor. Retain measurements on both sides of a joint when using the slab curling guide to distinguish shortening from vertical edge movement.

Distinctions

Free shrinkage
Length change measured with little external restraint. The measured contraction does not have to create a crack.
Restrained shrinkage
Contraction resisted by surrounding construction or reinforcement. Evaluating cracking also requires the restraint and the concrete's developing mechanical properties.

Field example

Two mixes tested at the same drying age report 0.048% and 0.064% contraction. The first has 25% less measured shrinkage: (0.064 minus 0.048) divided by 0.064. Over a freely shortening 30-foot length, the corresponding movements are about 0.173 and 0.230 inch. Neither result assigns that entire movement to one sawcut.

Frequently asked questions

Is 600 microstrain the same as 0.6% shrinkage?

No. Microstrain means millionths of length change per original length. Six hundred microstrain equals 0.0006 strain, or 0.06%, a factor of ten smaller than 0.6%.

Sources checked

Also defined as

  • The volume loss as hardened concrete dries, which cracks the concrete under restraint

Where this shows up

Next step: Track public floor projects