Plastic shrinkage crack

A plastic shrinkage crack needs a placement-time diagnosis: NRMCA CIP 5 attributes it to surface moisture escaping faster than bleeding replaces it while concrete is still plastic. Record first appearance, width, extent, and finishing stage together. Later discovery alone cannot establish when the crack formed. ASTM C1579-21's 0.5 mm control-crack criterion evaluates a laboratory fiber comparison; it supplies a test-validity threshold, separate from acceptance of the finished slab.

An early surface crack opened in the first hours when evaporation outruns the bleed rate

Used across 2 Anvilfield field guides, most in Concrete.
Updated

Record the pattern before the surface is repaired

NRMCA CIP 5's common crack spacing of 1 to 3 feet sets the photograph scale: include neighboring cracks, their ends, and a slab edge in the wide view. Add a close view with a width scale at a marked station. The two views connect a measured width to the pattern across the placement.

Put the crack stations on a bay or placement sketch with the first-observation time and the crew's finishing stage. Overlay the as-built top-bar locations as a separate settlement check when applying the crack diagnosis guide. A crack map, bar layout, and time record preserve more diagnostic evidence than a crack-family label alone.

ObservationRecord that survives finishing
Line visible during finishingPhotograph before closing it; mark the station and finishing stage.
Surface closed by refinishingRetain the original map and photograph the same station after hardening.
Crack first found the next dayRecord discovery time separately from formation time; retain earlier placement photographs.

Scope the repair from measured crack length

NRMCA CIP 5 identifies chemical ingress and initiation of later cracks as durability consequences even where these cracks rarely impair floor or pavement strength. Put the intended exposure and finish on the repair sketch. An appearance complaint, a liquid-tightness requirement, and continuing movement produce different repair scopes.

Four mapped crack segments measuring 18, 12, 7, and 9 feet total 46 linear feet for the repair takeoff. Keep the segment identifiers with that total so a revised scope can be remeasured. Surface length alone leaves treatment depth and product consumption unresolved; those quantities follow the selected repair detail.

After refinishing, return to the original stations and photograph them again after hardening. The before-and-after record preserves the location of a surface line that was closed during finishing and distinguishes it from a newly observed crack elsewhere in the bay.

Read the control result behind a fiber claim

ASTM C1579-21 requires an average control-specimen crack width of at least 0.5 mm for a meaningful comparison, with free-water evaporation rates within plus or minus 5% for each test. Retain both the control widths and the exposure record with the fiber result; a barely cracked control does not establish the required challenge.

With a control average crack width of 0.80 mm and a fiber-mixture average of 0.20 mm, the measured reduction is 75%: (0.80 minus 0.20) divided by 0.80, multiplied by 100. Report both widths beside the percentage. A 75% reduction from an unspecified baseline conceals whether the control met the test's minimum cracking criterion.

Match mixture identification, dosage, and test conditions when comparing fiber submittals. A changed water content or aggregate grading introduces another variable alongside the fiber. The comparison describes the tested mixture and fiber combination; its percentage does not forecast a crack count for the placement.

Distinctions

Control specimen
The reference concrete subjected to the same cracking exposure. It is part of the performance evidence, not merely a photograph beside the fiber panel.
Crack-reduction percentage
A relative result calculated from the stated control and test measurements. It is not a percentage reduction in structural design load or a guarantee of a crack-free slab.

Frequently asked questions

Is 0.5 mm an acceptable crack width for the finished slab?

No. In ASTM C1579-21, 0.5 mm is the minimum average crack width required in the laboratory control specimens to establish a meaningful comparison. It is not a field acceptance limit for an owner's concrete surface.

What should accompany a fiber crack-reduction claim?

The test method, mixture and fiber identification, dosage, control and fiber crack measurements, and exposure record. Those details establish the basis of the comparison and whether the submitted test matches the proposed mixture.

Sources checked

Where this shows up

Related guides

Next step: See public flatwork opportunities

Back to the full field glossary