Field glossary · property
Bleed water
Bleed water is mixing water displaced upward as the solid particles in fresh concrete settle. A useful bleeding measurement states how much water emerged, the exposed sample area, and elapsed time. Surface appearance alone misses water that evaporates as it arrives and water trapped beneath aggregate or reinforcement, so a dry-looking slab is not proof that internal bleeding has stopped.
Water that rises to the surface as solids settle, which protects the skin until it leaves or is removed
How concrete bleeding is quantified
ASTM C232/C232M-26 measures the relative quantity of mixing water that separates from freshly mixed concrete. ASTM C232/C232M-26 requires comparison samples of similar-density concrete to differ in mass by no more than 1 kg in the SI procedure. Use the inch-pound limits consistently when reporting under that unit system.
ASTM C232/C232M-26 describes a rodded specimen left undisturbed as representing concrete without intermittent vibration after placement. Repeatedly jarring a comparison bucket changes the condition being measured. Keep the consolidation method, collection times, sample temperature, and protection from evaporation with the result.
Convert collection volume to a comparable bleeding rate
For a measured collection interval, water-layer depth in millimeters = 10 × collected milliliters / exposed square centimeters. Divide that depth by elapsed hours to obtain millimeters per hour. State the interval: a rate averaged over the first half-hour is not the maximum rate within that half-hour.
Iowa State University's 2019 Integrated Materials and Construction Practices manual identifies section thickness and cementitious-material setting behavior as factors controlling bleeding duration. It also describes reduced bleeding with finer cement and increased cement content. A trial that changes cementitious fines therefore needs a new bleeding record, not just a new slump reading.
Keep a cumulative-volume plot as well as interval rates. A deep sample and a shallow sample expose different quantities of settling concrete beneath the same surface area. Compare specimens with the same geometry, consolidation and temperature so the curve describes the mixture change rather than the sample setup.
Find evidence below the surface
Bleeding channels and pockets under horizontal obstructions concern bond and local uniformity, whereas a surface puddle concerns the finishing face. When investigating a horizontal defect, compare its elevation with the reinforcing layout and placement sequence instead of assuming all separated water reached the top.
Pair the finishing timeline with the evaporation observations when interpreting a trial's water-delivery curve. Water emerging slowly under dry, windy conditions can disappear before a continuous surface film forms.
Distinctions
- Evaporation
- Water leaving the surface into the air. Visible accumulation is the balance between upward bleeding and outward evaporation.
- Cooling-tower bleed
- Intentional discharge of circulating water to control dissolved solids. It is a different use of the same word.
Field example
A covered sample with 500 cm² of exposed surface releases 50 mL over 30 minutes. The layer-depth calculation is 10 × 50 / 500 = 1 mm; dividing by 0.5 hour gives 2 mm/hour. That interval average is also 2 kg/m²/hour for water, allowing a comparison with an evaporation estimate expressed in those units.
Frequently asked questions
Can two mixes produce the same bleed volume at different rates?
Yes. Compare the time series as well as the final total; a slowly bleeding mix can continue supplying water after another mix with the same total has stopped.
Is a millimeter-per-hour result the same as percent bleeding?
The first is surface water delivery per area and time. Percent bleeding needs the collected water relative to the mixing water in the specimen; the area-based rate alone does not supply that denominator.
Sources checked
Also defined as
- Water that rises to the surface as solids settle; no finishing happens while it is present