Field glossary · property
Delamination
Delamination is a separation inside a material or between bonded layers, usually running approximately parallel to the surface. In concrete, the detached layer can remain in place and look intact. The diagnostic task is to locate the separation plane and identify which layer has lost support, because a thin finishing defect and a fracture above reinforcing steel require different repair quantities.
Separation within the concrete cover, often near corroding reinforcement; sounds hollow under chain drag or hammer before it spalls
Locate the separation plane before assigning a cause
A measured fracture plane 1/8 to 1/4 inch below the wearing surface fits the typical finishing-skin thickness described in NRMCA CIP 20. Compare that depth with the reinforcement and every overlay interface in a core through the marked area. Assigning corrosion as the cause without locating the fracture plane can turn a thin resurfacing quantity into an unjustified cover-removal scope.
Log the interface depth from the existing wearing surface and identify every layer penetrated. If an overlay remains attached to a detached substrate, testing only the overlay-to-substrate bond misses the failing plane beneath it. The repair boundary must follow the material that remains sound, not the coating edge visible from above.
What a hollow sound can and cannot establish
FHWA's concrete sounding guidance identifies hammer sounding as a method for significant shallow delaminations and states that it does not detect early-stage or deep delamination reliably. A solid response is therefore a finding for that method and location, not proof of an entirely defect-free section.
FHWA advises against sounding frozen concrete because the condition interferes with interpretation. Background traffic noise also reduces the usefulness of an audible comparison. Record those conditions, use nearby sound material as a reference, and preserve uncertain areas for another method rather than erasing them from the map.
When reviewing a troweled floor's batch records, use NRMCA CIP 20's recommended 3% maximum air content as one clue to finishing-related delamination. Compare air content with the fracture depth and finishing history. Exterior freeze-thaw mixtures have a different durability requirement, so this floor recommendation cannot decide their air target.
Turn a defect map into a repair quantity
A survey marks 180 square feet of hollow response, including 25 square feet already broken open. The initial mapped footprint is 180 square feet, not 205: the visible spalls are inside the hollow-area total. Keep separate columns for mapped area, confirmed removal depth, and additional unsound concrete found during breakout.
Depth changes the investigation. A shallow separation directs attention to flatwork finishing, while a fracture following reinforcement supports the corrosion assessment used in parking-structure restoration. Record that distinction beside the mapped quantities.
Distinctions
- Spalling
- Spalling is actual loss of material from the surface. A delaminated layer can remain attached at its perimeter before it breaks away.
- Blister
- A blister is a localized raised pocket. Delamination can extend across a much broader area without an obvious raised surface.
Frequently asked questions
Does hollow concrete always mean corroded rebar?
No. A finishing skin, an overlay interface, or a separation within the cover can all sound hollow. Identify the fracture plane before assigning the repair cause.
Can a coating adhesion test locate every delamination?
A local adhesion result describes the tested specimen and its failure plane. Sounding and selected deeper verification establish the surrounding extent.
Sources checked
Also defined as
- Paving: Separation of an asphalt layer from the one below at the bond line, often breaking up into potholes
- A separation within the concrete, often at the reinforcing, that sounds hollow before it falls