Field glossary · process
Carbonation
Report carbonation as a depth tied to local reinforcement cover: carbon dioxide consumes alkaline cement compounds, and an indicator reveals the resulting change in alkalinity. An 18 mm colorless zone with 25 mm bar cover leaves 7 mm between the visible boundary and the steel. The Concrete Society places possible steel depassivation a few millimeters ahead of that boundary, so the reagent and test method belong beside the paired depth readings.
Loss of concrete alkalinity as carbon dioxide reacts in over time, which depassivates the steel
What a phenolphthalein boundary actually measures
BSI lists BS EN 14630:2006 as the current standard for determining carbonation depth in hardened concrete by the phenolphthalein method. The measurement follows an alkalinity change in the cement paste. Aggregate particles that remain uncolored are not, by themselves, evidence that the surrounding paste has carbonated.
FHWA's 2002 laboratory guidance uses a 0.5% phenolphthalein solution in methanol for carbonation staining. In that method, FHWA identifies paste above pH 10 by its magenta response, while carbonated paste and other constituents remain unstained. Record the actual reagent and method instead of treating every pink-and-clear photograph as the same test.
The Concrete Society notes that steel depassivation can occur a few millimeters ahead of the phenolphthalein color boundary. A thin colored strip between the apparent front and a reinforcing bar is therefore not a precise measure of remaining corrosion protection.
Pair depth and cover at the same exposure
Organize the survey by exposed face and moisture condition. A sheltered soffit result and a rain-washed vertical-face result belong to different locations even when both come from the same member. Keep the original exposed face identifiable on every split core or broken sample, then measure inward from that face through the paste.
Give each paired result a location identifier on the elevation drawing. Carbonation observations and cover readings from the same bar neighborhood support a repair boundary; separate averages for an entire elevation conceal local shallow cover. Carry that location map into the removal scope developed with the concrete repair guide.
| Survey record | Interpretation it preserves |
|---|---|
| Face, location, and sample orientation | Which exposed surface the penetration depth starts from. |
| Indicator, preparation, and reading time | How the photographed boundary was obtained. |
| Boundary depth and local reinforcement cover | Whether the measured zone approaches or overlaps the steel. |
| Cracks, wetting, rust staining, and adjacent tests | Evidence needed to separate reduced alkalinity from active deterioration. |
Read the remaining cover without inventing a service life
At a balcony edge, a measured colorless depth of 18 mm and local bar cover of 25 mm leave 7 mm between the visible boundary and the steel. At an adjacent shallow-cover location with 15 mm cover, that same depth extends 3 mm beyond the steel position. The second location deserves separate treatment in the condition map even if the elevation's average cover looks satisfactory.
Those subtractions locate the observed front; they do not establish its travel speed. Converting the 7 mm separation into years requires exposure history and a calibrated progression model. Use dated repeat observations at identified locations to determine movement of the boundary, and use corrosion measurements to establish what the reinforcement is doing now.
Frequently asked questions
Does pink concrete mean the reinforcing steel is corrosion-free?
Pink indicates the reagent's alkaline response. It does not exclude chloride-induced corrosion, and it does not place the depassivation boundary exactly at the visible color transition.
Can carbonation depth be read from an old exposed break?
Use a freshly exposed surface or split core. An old break has acquired its own exposure to air, so its color response can describe alteration after the break rather than penetration from the original concrete face.
Sources checked
Also defined as
- CO2 reacting with the paste and lowering concrete pH, de-passivating the steel at the front