Field glossary · measurement
Slump flow
Slump flow is the average of an SCC patty's longest diameter and the diameter perpendicular to it, measured after flow stops. WAQTC's 2025 procedure invalidates a test when those readings differ by more than 2 in. A 27.5 by 24.5 in. patty therefore cannot be reported as a valid 26.0 in. flow. Keep both original diameters: the average alone hides a failed geometry check.
Average spread diameter of the SCC patty after the cone lifts, the SCC measure of filling ability
When an average spread is not a valid result
WAQTC's 2025 field procedure for AASHTO T 347/T 351 requires repeating the slump-flow test when the two measured diameters differ by more than 2 in. [50 mm]. It identifies sideways movement during cone removal as a likely cause. This checks the geometry of the test itself, before the average is compared with the specified flow.
A patty measuring 27.5 in. by 24.5 in. averages 26.0 in., but its 3.0 in. diameter difference invalidates the test under that procedure. Another patty measuring 26.5 in. by 25.5 in. has the same 26.0 in. average with a 1.0 in. difference. Only the second clears this particular geometry check; the flow target and other required properties still need their own results.
Measure the whole patty and keep the lift consistent
WAQTC's procedure first selects the largest diameter, then its perpendicular diameter, measuring each to the nearest 1/4 in. It includes any mortar border or bleed-water halo in the measurement. Two arbitrary perpendicular axes can miss the largest mismatch and wrongly clear the 2 in. validity limit. Keep the full edge-to-edge readings and describe visible separation independently.
WAQTC specifies lifting the mold in 3 ±1 seconds for its SCC procedure. Use that SCC lift window when timing the operation or training a technician. Record the method designation so the equipment setup and reported values can be traced to the procedure actually performed. ASTM C1611/C1611M-21 remains the current ASTM slump-flow method.
Aggregate size and the limits of an open spread
ASTM C1611/C1611M-21 describes its method as applicable to SCC containing coarse aggregate up to 1 in. [25 mm]. Its Appendix X1 visual-stability criteria and relative-viscosity procedure are nonmandatory. WAQTC's cited FOP, by comparison, includes the VSI determination in its procedure. Name the governing method before deciding which observations belong in the report.
A record for SCC placement should identify which result is the open flow and which comes from an obstruction test. The 2 in. within-patty geometry check does not set a J-ring acceptance limit or establish an allowable reinforcement spacing. Those are separate comparisons with different physical meanings.
Distinctions
- Diameter difference versus J-ring difference
- A diameter mismatch can invalidate the operator's spread test before any passing-ability decision. Substituting the J-ring result for the missing valid open-flow result would combine a material comparison with an unresolved test defect.
- T50 versus final spread
- WAQTC records T-50 when the patty first touches the 20 in. reference circle in its inch-pound procedure, or the 500 mm circle in its SI procedure. Equal final spreads can have different T-50 times; record the time separately from the final diameter.
Frequently asked questions
Should I leave the mortar halo out of the diameter?
Include it when using the cited WAQTC procedure. Record its presence with the stability observation rather than adjusting the spread to make the concrete appear more uniform.
Can I report collapse as a very high ordinary slump?
Use the method specified for the mixture. The concrete slump guide explains the switch to SCC testing; a collapsed ordinary slump specimen does not provide a measured spread diameter.
Sources checked
Also defined as
- The spread diameter of self-consolidating concrete, measured per ASTM C1611 instead of slump