ANVILFIELD Try FieldOS

ASTM International

ASTM C876: half-cell cutoffs, reference cells and repeatability

Half-cell surveys under ASTM C876-22b locate differences in reinforcement potential against a reference electrode. ASTM International publishes the method for uncoated steel. Read each map with its electrode identity, contact coordinates and environmental record, then separate repeatability from corrosion interpretation. Repair quantities need corroborating investigation because a potential reading does not measure steel loss.

Current edition: ASTM C876-22b (2022)
Updated

Official publisher page

Applies to

An estimator preparing a C876-22b survey should schedule membrane-covered test faces and epoxy-bar zones as separate investigation work. ASTM’s exclusions keep those zones out of an ordinary potential-mapping quantity. Have the owner identify the reinforcement system and accessible concrete faces before the testing firm sets its grid and field allowance. A total deck area alone does not establish the area this method can survey.

Key topics

Apply corrosion-potential bands to a recorded electrode basis

A record containing -180, -275 and -410 mV versus copper/copper sulfate crosses the three screening bands in Proceq’s PM8500 manual, revision 4.0 (October 2025), which identifies them as C876-22b Appendix X1 criteria. The -180 mV point lies above -200 mV, in the 90% probability band for no active corrosion; -410 mV lies below -350 mV, in the 90% active-corrosion band. The -275 mV point is uncertain. These interpretations apply under conditions suitable for the C876 potential criteria. Pair each classification with the reference electrode and corroborating investigation, even when its same-point repeat passes.

Repeated readings and different electrodes are separate checks

ODOT’s 2014 Cathodic Protection Evaluation, discussing ASTM C876-09, gives a 10 mV maximum difference for repeated readings at the same location with the same reference electrode and 20 mV for readings with two different reference electrodes. These published comparison benchmarks address different sources of disagreement. Record which electrode and exact point produced each result. A reference-cell comparison performed in a controlled setup is a different record from a repeat on the structure, where surface contact and point location also enter the measurement.

A small location error can imitate instrument drift

ODOT’s report reproduces an Alsea Bay Bridge potential map with a change exceeding 300 mV in less than 1 ft. A repeat moved along that gradient can differ substantially even with a stable instrument. Register the electrode contact position to a recoverable mark, and distinguish a deliberate adjacent reading from a same-point repeat. When readings disagree, retain both coordinates and values before averaging. The repair guide’s investigation map then receives the local gradient rather than a smoothed result that hides it.

Temperature and deep cover can obscure a survey change

ASTM C876-22b identifies 22.2°C ± 5.5°C, or 72°F ± 10°F, as the range in which temperature influence can be neglected; measurements outside it need temperature dependence accounted for. ASTM also notes that cover exceeding 75 mm, or 3 in, can average adjacent potentials and reduce spatial discrimination. Record temperature and cover with the map. A broad, smooth contour under deep cover does not carry the same spatial resolution as a sharp gradient measured through shallow cover.

How it is used in the field

Specify the deliverable as a recoverable dataset with a repeat log, not only a colored contour drawing. Each repeated observation needs the original point identifier, electrode identity, original and repeated potentials, elapsed time and reason for repetition. Assign different identifiers to adjacent checks. This distinction makes a later reviewer’s disagreement traceable to a measurement, a coordinate or an interpretation.

A same-electrode repeat of -312 and -325 mV at one marked point differs by 13 mV, exceeding ODOT’s historical 10 mV comparison benchmark. A pair of -312 and -318 mV differs by 6 mV. Resolve the disagreement in the first pair before calling it a time trend. Passing the second comparison establishes repeatability for that pair, not a corrosion rate or a remaining bar diameter. Label the ODOT 2014/C876-09 benchmark explicitly when it is specified alongside the current C876-22b method.

Connect suspect gradients to selected physical and chemical investigation locations. ASTM C876-22b identifies chloride, carbonation, delamination, corrosion-rate and exposure information as complementary evidence. The concrete diagnostic test guide assigns each of those methods its own question. Preserve a gradient that warrants investigation even when a rounded site average appears unremarkable.

Frequently asked questions

Can the copper/copper sulfate cutoffs be used with any reference cell?

Keep the reference-cell basis attached to the voltage. The FHWA screening bands used here refer to the copper/copper sulfate setup. Results from a different reference-electrode system need interpretation on that system’s basis before maps or numerical cutoffs are compared.

Does a stable reading establish residual reinforcing capacity?

ASTM C876-22b excludes estimating structural properties from its results. Stable readings establish a usable potential measurement; remaining steel dimensions and structural analysis answer the capacity question.

Sources checked

Sections and parts cited

ASTM C876-09

Field guides that apply ASTM C876

Browse all codes and standards