Field glossary · method
Notched-wedge joint
A notched-wedge asphalt joint needs a cross section showing both notches and the tapered overlap that the next paving pass will cover. Calculate width from the vertical drop remaining between the notches, rather than selecting a width alone. For a 60 mm lift with two 12.5 mm notches, a 6:1 taper occupies 210 mm horizontally; the lift and aggregate size control whether that detail fits.
A tapered longitudinal joint with small top and bottom notches, formed by a screed shoe to confine the first pass edge and densify the seam
Resolve the vertical dimensions before choosing a width
The Asphalt Paving Handbook section 9.3.1.3 recommends notches at both the top and bottom of the wedge, each at least one nominal maximum aggregate size deep. The top notch, sloping face and lower notch share the available lift thickness.
In a 60 mm finished lift using 12.5 mm NMAS mix, two 12.5 mm notches leave 35 mm of vertical drop for the taper. Multiply that remaining drop by the horizontal-to-vertical ratio to obtain wedge width. The dimensions below describe that cross section, not a one-foot attachment setting.
| Taper for a 35 mm drop | Horizontal wedge width |
|---|---|
| 6:1 | 210 mm |
| 4:1 | 140 mm |
A taper range is not a single standard detail
FHWA-HIF-21-023 describes notched-wedge configurations with slopes from 3:1 to 12:1. The report identifies the notch as important because a taper running to zero thickness can drag larger aggregate.
Specify the accepted profile, then identify whether measurements describe loose material or the compacted edge. The two construction stages have different elevations. Set the shoe against the intended stage and use the joint construction guide to coordinate the adjacent pass.
Check the wedge that will disappear under the next pass
FHWA-HIF-21-023 notes that research has raised concerns about limited compaction within the wedge itself, even where the wedge provides confinement that benefits the joint. Inspecting only the completed surface can miss the condition of the buried taper.
Record wedge geometry and compaction before covering it, together with the station limits of any disturbance or replacement. The joint-maker entry distinguishes a forming shoe from equipment that also applies compactive effort. The longitudinal-joint entry explains why the eventual sampling location must account for the buried wedge rather than only the visible seam.
Distinctions
- Unnotched taper
- A taper that terminates at a feather edge provides a different aggregate-placement condition. A sloping appearance alone does not establish a notched-wedge profile.
- Pavement-edge safety treatment
- A taper at the outside edge of a roadway serves a different location and purpose from an interface intended to be covered by an adjacent asphalt pass.
Frequently asked questions
Can a wedge detail be reduced proportionally for a thinner lift?
Proportional scaling also reduces notch depth. The Asphalt Paving Handbook’s one-NMAS notch depth is a recommendation; the project detail establishes the required geometry. Compare that detail with the new aggregate size and remaining lift depth before reusing the shoe setting.