ASTM International
ASTM C39: loading rate, cylinder geometry and laboratory reports
Cylinder compression testing under ASTM C39/C39M-26 depends on measured geometry, suitable bearing surfaces and a controlled stress rate. The method also covers drilled cores and is limited to concrete denser than 800 kg/m³, or 50 lb/ft³. A laboratory result needs enough detail to establish how the load was applied and calculated. The test method produces a strength measurement; the project’s acceptance framework determines the decision made from it.
Applies to
Laboratory technicians perform C39, equipment managers maintain the loading system, and engineers and inspectors review the results. Tie specimen identifiers to the fresh-concrete sample record before testing. Keep the strength-testing guide's load-to-area calculation auditable with the measured dimensions, end preparation and loading record.
Key topics
Stress rate is not the same as force rate
FDOT’s September 2014 C39 procedure checklist specifies 35 ± 7 psi per second during the latter half of the anticipated loading phase. The machine’s required force rate therefore depends on specimen area. Record the selected units and control mode when setting up the machine. A force-rate setting appropriate to one diameter does not preserve the stress rate for a different cylinder size.
Use the measured diameter in the area calculation
FDOT’s checklist averages two perpendicular diameters measured near mid-height and records diameter to the nearest 0.01 inch. The actual measurement supplies the cross-sectional area. Using a nominal mold diameter in every calculation hides dimensional variation and can move the reported strength. Keep both observed diameters in the laboratory worksheet rather than retaining only the rounded strength.
Repair an unsuitable bearing surface before loading
FDOT's checklist screens the specimen ends for 0.002-inch planeness and alignment against 0.5 degree. FHWA's hardened-concrete laboratory manual explains the response to an uneven end: saw or grind it to tolerance, or use the applicable C617 bonded-cap or permitted C1231 unbonded-cap system. Keep the end-treatment record with the specimen dimensions. A favorable maximum load cannot establish that bearing preparation was acceptable.
How it is used in the field
For a cylinder with a measured 4.00-inch diameter, area is 12.566 square inches. A target of 35 psi per second therefore requires about 440 pounds-force per second. At 6.00 inches, area is 28.274 square inches and the same stress rate requires about 990 pounds-force per second. Applying 990 pounds-force per second to the smaller specimen would impose about 79 psi per second, well above the cited 28-to-42 psi-per-second range.
A 50,000-pound failure load divided by the area of a measured 3.95-inch diameter gives approximately 4,080 psi. Substituting the nominal 4.00-inch diameter gives approximately 3,980 psi. The roughly 100 psi difference comes from the input geometry, before any question about mixture performance. Preserve the load and dimensions so the reviewer can reproduce the calculation.
For a drilled core, carry the sampling identity and preparation information from the core assignment into the compression report. C39 covers the loading measurement; it does not replace the requirements for obtaining and preparing the core. The slab acceptance guide explains where core evaluation enters an investigation. Keep that evaluation decision separate from the laboratory’s individual test result.
Link each result to specimen dimensions, end preparation, test age, maximum load, fracture observations, machine identity and operator. ASTM C39/C39M-26 requires acceptance-testing technicians to satisfy C1077, including an independently evaluated performance demonstration. Its safety warning also calls for containment of concrete fragments during sudden failure. Verify the machine's fragment enclosure before loading and retain each specimen's result before calculating the group average.
Adoption
FDOT publishes a dedicated independent-assurance checklist for the C39 compression test. Its dated checklist supplies the public agency controls cited here; the laboratory’s controlled procedure identifies the edition required for the current assignment.
Frequently asked questions
Does C39 require a 28-day test on every project?
The assigned test age comes from the testing program and specification. C39 governs the compression measurement at that age. Record the required and actual age so a properly run test is not used for the wrong scheduled decision.
Can a light insulating-concrete cylinder be tested under C39?
Check the density and material assignment. C39/C39M-26 is limited to concrete above 800 kg/m³ [50 lb/ft³]; the low-density insulating-concrete program needs its applicable material-specific test method.