ANVILFIELD Try FieldOS

ASTM International

ASTM C231: pressure meter calibration and aggregate correction

Pressure-method air content under ASTM C231/C231M-26 requires a suitable aggregate, a calibrated meter and an aggregate correction factor. The gauge reading alone is not necessarily the concrete’s air content. The method applies to plastic concrete with relatively dense aggregate whose correction can be established; lightweight, highly porous and air-cooled slag aggregates fall outside that scope. Meter calibration and aggregate correction solve different errors and need separate records.

Current edition: ASTM C231/C231M-26 (2026)
Updated

Official publisher page

Applies to

Concrete testing technicians perform the measurement, while agency reviewers and producers need evidence that the instrument and correction match the mixture. A pressure-air result enters the fresh-concrete testing record with two supporting files: the meter’s calibration history and the aggregate-factor determination for the sampled mixture.

Key topics

An aggregate correction factor is not a gauge adjustment

ASTM C231/C231M-26 requires determination of the aggregate correction factor because the test must exclude the response of air inside aggregate particles. Iowa DOT IM 318 determines that response with aggregate matching the mixture’s proportions and moisture condition, soaked for approximately the same interval as the concrete before testing. A new aggregate source is therefore a material change to review, even when the meter has just passed calibration. Iowa also rounds its aggregate correction down to the nearest 0.5 point; that agency convention must not be silently imported into an ASTM-only worksheet.

Check zero and a known air volume separately

Iowa DOT IM 318 calls for annual calibration, a calibration check before project use and periodic checks during the construction season. Its water-filled zero check establishes the initial pressure setting. A known-volume canister then checks the scale response. Passing zero alone does not demonstrate that the meter reads correctly at the air content used for acceptance.

What an Iowa calibration tolerance actually checks

Under Iowa IM 318, a 0.0125-cubic-foot canister simulates 5.0% air in a 0.250-cubic-foot bowl. A one-canister reading differing by 0.2 percentage point or more triggers the two-canister check, which represents 10.0% in that bowl. The agency's scale tolerance is 0.2 point, or 0.25 point for a dial with 0.5-point divisions. Record the bowl volume and both applicable check readings; these are meter criteria, separate from the concrete's specified air band.

How it is used in the field

A 7.2% dial reading with an established 0.5-percentage-point aggregate correction gives 6.7% concrete air: 7.2 - 0.5. If the project band is 5.0% to 7.0%, the corrected result falls inside it although the raw reading is above it. Retain the dial observation, factor and calculated result. Reporting only 7.2% would reverse this acceptance comparison.

A meter expected to read 5.0% with the calibration canister instead reads 5.4%. The 0.4-point discrepancy exceeds the cited Iowa tolerance. Do not compensate by changing the aggregate factor: that would disguise an instrument problem as a material property. Follow the agency’s repeat-check and instrument-adjustment process, and document the meter’s return to service before using it for acceptance results.

Assign an instrument identifier to each result so a later failed check can be traced to the affected observations. Keep the calibration date and known-volume results in the equipment file and the aggregate-factor determination in the mixture file. This separation makes it possible to resolve whether an unexpected air trend follows one meter, one aggregate source or both.

Adoption

Iowa IM 318 is an agency pressure-air procedure referencing AASHTO T 152. Its calibration details provide a documented agency application alongside ASTM C231; the project testing specification identifies which procedure governs the reported result.

Frequently asked questions

Can an aggregate correction make pressure testing suitable for lightweight concrete?

No. C231/C231M-26 excludes lightweight and highly porous aggregates and directs those concretes to C173/C173M. A guessed correction does not extend the pressure method’s material scope.

Is Iowa’s annual calibration interval an ASTM-wide service rule?

It is the interval stated in Iowa IM 318. Identify the governing agency procedure and laboratory equipment program for the job rather than assigning a regional interval to every C231 project.